Nickel Institute
Corrosion by Process Waters R. W. Ross Consultant Nickel Institute
Summary Scaling and Corrosion Effects of Velocity Biological Effects Chlorides Rouging of SS
Water Chemistry Effects Corrosion Dissolved Oxygen Chlorides pH Hardness Temperature Scale Dissolved Solids Calcium Ions pH Temperature
Water Chemistry Effects
Corrosion Of Carbon Steel In Water 0.76 72 ºF (22 ºC) 104 ºF (40 ºC) 0.51 Corrosion Rate, mpy Corrosion Rate, mm/y 0.25 pH of Water
Corrosion Of Carbon Steel In Low-velocity Water
Corrosion Of Carbon Steel Effect Of Velocity In Seawater 1.27 Corrosion Rate, mpy Corrosion Rate, mm/y 0.64 (1.5) (3.0) (4.7) (6.1) (7.6) ft/sec (m/s)
Erosion-corrosion - Inlet
Erosion-corrosion Flow
Erosion-corrosion Tube Blockage Flow
High-velocity Seawater >120 fps (36.6 m/s) Corrosion Rate, Alloy mpy mm/y 625/C-276 <1 < 0.03 400/K-500 <1 < 0.03 718/725/925 <1 < 0.03 T-304/T-316 <1 < 0.03 C Steel >300 > 7.62
Biological Effects Macrofouling Mussels Clams Barnacles Plant Life
Biological Effects Macrofouling
Bacteria Effects - MIC (Microbiologically Induced Corrosion) Species Oxygen Metals Corrosive Desulfovibrio No Fe, Al, Cu Sulfide Thiobacillus Yes Fe, Cu Sulfuric Acid Gallionella Yes Fe Fe++ to Fe+++ Mn++ to Mn+++
Bacteria Effects - MIC Type 304 SS water tank 8 months of service Guam
Bacteria Effects - MIC (Type 304 SS, Before Cleaning)
Bacteria Effects - MIC (After Cleaning) 0.15 in. (3.8) mm) Max. Attack
Bacteria Effects - MIC (After Cleaning - No Attack)
Prevention Of MIC Keep The System Clean Keep Water Flow > 6 fps (2 m/s) Use Bactericide: Chlorine Chlorine Dioxide Hypochlorite Ozone Non-oxidizing
Prevention Of MIC Use Continuous Cleaning Use High Pressure Hydrolancing Use Stainless Steel Scrapers (Hard to Remove or Heavy Deposits) Use Alloy Resistant to MIC
Prevention Of MIC - 6% Mo ALLOY
Effects of Chlorides
Crevice Corrosion Type 303
Stainless Steels Localized Corrosion Resistance Alloy PRE 304 18 316 25 317 30 2205 34 2505 37 2507/Alloy 100 41 6% Mo Alloys 40 - 45
Nickel Alloys Localized Corrosion Resistance Alloy PRE 316 25 6% Mo 40 – 45 625 52 22/622 65 C-276 69 2000 76 686 76 59 76
Stainless Steels for Use in Waters Potable water Type 304 < 200 ppm chlorides Type 316 < 1000 ppm chlorides River water Risk of MIC if water is not treated Use type 316 or higher Mo grades: 2205 904L 2507 6Mo Well water Use type 316 or higher Mo grades
Do not confuse Chloride Cl- and Chlorine Cl2 Maximum Concentration (ppm) in Water to Avoid Crevice Corrosion Chloride Cl- Chlorine Cl2 304 200 2 316 1000 4 Shock dosing, such as 25 ppm chlorine for 24 hours, is common practice and has not been found to cause problems.
Stress Corrosion Cracking (SCC) Steam Line
Chloride SCC Duplex vs T-316 Stainless Steel No cracking below lines Type 316 (315) 22 Cr Duplex 18 Cr Duplex (204) (93)
Effect of Nickel Content on Stress Corrosion Cracking Boiling 45% MgCl2 No SCC Ni Alloys SCC 6% Mo SS Duplex SS
HIGH CHLORIDE WATERS
How does external environment affect process equipment? HIGH CHLORIDE WATERS How does external environment affect process equipment?
Marine Corrosion of C Steel Relative Corrosion Rates Marine Corrosion of C Steel Relative Corrosion Rates* – Vary with Sea Conditions Atmospheric Splash Tidal Submerged Subsoil *Protected Harbor 25 mpy (0.64 mm/y) 5 mpy (0.13 mm/y)
Uniform Corrosion
Effect of Chromium Weight Loss, mg. / sq. dm. 250M Lot 44 Months
Alloy C in Marine Atmosphere 56 Years of Exposure
Type 304 Fastener In Marine Tide After 6 Months
Type 304 Fastener Above Marine Tide After 6 Months
Crevice Corrosion
Crevice Corrosion of Alloy 825 Heat Exchanger Tubing – Shell Side 85° F, Aerated Seawater
Crevice Corrosion of Alloy 625 Waterbox With Deaerated, Treated Seawater
Crevice Corrosion of Alloy 825 Heat Exchanger Tubesheet – Water Side 225° F, Deaerated, Treated Seawater Tube to Tubesheet Joint
Types Of Severe Crevices Stationary O Rings Non-Metallic Connector Flange Face Under Gasket Tube to Tubesheet Joint
Corrosion of 90-10 Cu-Ni in Seawater Corrosion Rate, mpy
Marine Fouling 18 Months in Quiet Seawater C Steel Aluminum
Fouling of Titanium Waterbox 3 mo. Exposure
Fouling of Titanium Waterbox 6 mo. Exposure
Effect of Chlorination <1 fps Seawater Flow
90-10 Cu-Ni Alloy Fouling - Quiet Seawater 3 Mo 9 Mo 18 Mo 3 Yr 4 Yr 5 Yr
90-10 Cu-Ni Intake Piping Desalination Plants
Seawater Piping Systems 90-10 Cu-Ni Alloy Seawater Piping Systems
Seawater Heat Exchangers 90-10 Cu-Ni Alloy Seawater Heat Exchangers
Pumps - Impellers
Rouging of Stainless Steels High Purity Water Water For Injection (WFI)
Why Use Stainless Steels (316L) for Pharma & Biotech? Good corrosion resistance and excellent batch to batch cleanability Good structural properties for process equipment Easily formed, fabricated and welded
What about Rouging. What is Rouging What about Rouging? What is Rouging? Rouging is a general term used to describe several species of predominately iron oxide deposits on the wall of piping and vessels in high purity water systems.
Rouging is not New! Rouging is not unique to the pharmaceutical and biotech industries. Was recognized over 40 years ago with rouging of SS vessels at Savannah River.
Where is Rouge often Found Water systems, usually high purity water and clean-steam systems Distillation and clean-steam generating equipment Rouge found on wall of vessels, piping and polymer gaskets (Teflon®) downstream of where originated
Is Rouge Harmful? No reports or evidence that rouging is precursor to a SS corrosion failure. We are not in a position to comment on whether rouge is harmful to the product being produced. Common practice is to remove rouge.
Rouging Generally a loose powdery deposit, but can be tightly adherent Hydrated or partially hydrated ferric oxide (Fe2O3) or ferroso-ferric oxide (Fe3O4) Usually occurs in high purity (0.5-1.0 µS/cm), high temperature water (60 – 100 C)
Rouging Reddish brown rust color, but can range from orange to blue-black. Origin is uncertain but generally thought to be ions or colloids that are formed at one location and transported in the solution to another where they are precipitated. Removed by acid cleaning in nitric, phosphoric, citric, or oxalic acid.
Rouging - Types Type 1 – Corrosion of Steel, Deposits Downstream Pumps prime suspects – cavitation or erosion when velocity over ~ 100fps and higher temperatures Delta ferrite in cast impellers may contribute by eroding easier and higher iron content Type 2 – Corrosion Product of Stainless Steel Type 3 – Corrosion Product of Stainless Steel in Steam Systems > 100 C
Rouging of Stainless Steels
Rouging over 4 years inside electropolished Type 316L - column still used to produce ultra-pure water for pharmaceutical use
Rouging of Stainless Steels
De-rouging & Passivation 3 Steps Cleaning – detergent wash followed by thorough water rinse De-rouging chemical treatment Passivation followed by thorough water rinse
Electrochemical Coloring Proprietary electrochemical processes – invented in 1972 by Inco, further developed in Japan Interference between the light beams refracted from the substrate and the surface of the oxide film creates color Appearance and color vary with immersion time and surface finish Incident light Color Oxide
Experience Music Project
Summary Discussed Scaling and Corrosion Described Effects of Velocity Reviewed Biological Effects Discussed Chlorides Summarized Rouging of SS
Questions ?