Flotation of Cu-Au, PGM and Cu-Mo
Group 1 Taylan Berkkam Bedrettin Ozakyuz Cem Sarikaya Ertuna Cakir Lecturers: Prof. Dr. Zafir Ekmekci and Asst. Prof. Ozlem Bicak
2
ACACIA Mining Bulyanhulu Au-Cu Flotation
TANZANIA
3
Run of Mine Upper East Zone 3g/t Au, 0.2% Cu
Lower Mine 10g/t Au, 0.5% Cu
4
Ore Content Chalcopyrite (Cu) Auriferous Pyrite (Au) Native Gold
5
Aim Floating Chalcopyrite Discarding Pyrite Gravity Separation
6
Flowsheet Rougher Cleaner PAX-Aerophine as Collector Aerophine
Betafroth frother Lime pH 11-12 pH Betafroth Carboxyl methyl cellulose (CMC)
7
PGM Minerals There are more than 100 PGM minerals.
These minerals are subjected to a wide range of elemental substution. These sulphide deposits are able to concentrate these metals by a factor of 100–1000 ppm and form PGM deposits, together with precious metals, nickel and copper. Almost always the PGM deposits contain nickel minerals.
8
PGM Dominated Deposits
Morensky type deposits Hydrothermal deposits Place deposits
9
Effect of Mineralogy on Recovery of PGMs
From a processing point of view, PGM-containing ores can be divided into three general groups as follows: ores amenable to gravity pre-concentration, ores amenable to flotation ores that can only be treated using a hydrometallurgical route.
10
Ores Amenable to Flotation
Based on flotation processing characteristics, these ores can be divided into the following major groups: PGM sulphide-dominated deposits PGE-dominated deposits
11
Flotation of PGM Containing Ores
Flotation properties of PGM from sulphide dominated deposits Pyrrhotite Chalcopyrite and pentlandite Violarite
12
Reagent Practice in Flotation of PGM Sulphide-dominated Ores
Activators Collectors Depressants CuSO4 (CMC) Carboxymethyl Cellulose Oxalic Acid and Thiourea Primary Xanthate(SIBX) Secondary Dithiophosphates & Mercaptans Guar gum pH=9-10
13
Flotation of Sulphide Dominated Ores
There can be some variation in this flowsheet, such as (i) retreatment of the cleaner tailings, (ii) regrinding the scavenger concentrate and iii) the number of cleaning stages. This flowsheet is used in several operations from the Bushveld Complex (South Africa), Stillwater Complex (USA) and Lac des Illes (Canada).
14
Reagent Schemes Used to Treat PGM Containing Ores
15
Copper Molybdenum Flotation
Application Field Of Molybdenum 80% of Mo are being used in steel industry; to increase mechanical properties of steel and to produce stainless steel. 20% of Mo are being used in some chemical applications. in addition, saleable Mo concentrate must include at least 50% of Mo and not exceed 0.5% of Cu in Mo Concentrate
16
The study of low-grade porphyry copper-molybdenum ore obtained from the Kirklareli region of Turkey
The Effect of Grinding
17
The study of low-grade porphyry copper-molybdenum ore obtained from the Kirklareli region of Turkey
The Effect of pH
18
The study of low-grade porphyry copper-molybdenum ore obtained from the Kirklareli region of Turkey
The same experiment with Na2S At pH 6 At pH 12
19
The study of low-grade porphyry copper-molybdenum ore obtained from the Kirklareli region of Turkey
Effect of Frothers
20
The study of low-grade porphyry copper-molybdenum ore obtained from the Kirklareli region of Turkey
Depressant Selection Effect of Sodium Sulfide Effect of Nokes Phosphorus Pentoxide-Sodium Hydroxide
21
The study of low-grade porphyry copper-molybdenum ore obtained from the Kirklareli region of Turkey
Effect of lignosulphonate Sodium Metabisulfite
22
The study of low-grade porphyry copper-molybdenum ore obtained from the Kirklareli region of Turkey
Effect of Sodium Cyanide
23
The study of low-grade porphyry copper-molybdenum ore obtained from the Kirklareli region of Turkey
Effect of Collectors
24
The study of low-grade porphyry copper-molybdenum ore obtained from the Kirklareli region of Turkey
Conclusion Molybdenum Flotation:The selective molybdenum flotation has carried out at pH value of 12 , Na2SiO3 as silicate depressant , 10 g/ton Na2S as copper depressant , 440 g/ton kerosene as collector and 56 g/ton pine oil as frother. Copper Flotation: The selective copper flotation has carried out at pH value of 12 , 100 g/ton Aero 3302 as collector , 28 g/ton pineoil. Reference Kırklareli Demirköy-Sivriler Molibden Cevherinin Flotasyon ile Zenginleştirilmesi. Şükriye Beste EVEN (05 Haziran 2009)