Curious stress reduction with W incorporation of WC-C nanocomposite films by hybrid ion beam deposition A. Y. Wang a), H. S. Ahn a), K. R. Lee a), J. P. Ahn b) a) Future Technology Research Division, b) Nano-materials Research Center, Korea Institute of Science and Technology. KVS ---- 2004.08.19
2
Heart valve Watch bracelet Hard disk MEMS package Spur gear Properties of DLC hardness up to 4000 HV deposition temperature ca. 100 °C temperature stability < 350 °C tribology low friction and wear stable against acids and alkalines biocompatible, haemocompatible Hip joints Introduction
3
Key obstacle to applications Urgent dillemma: how to reduce stress without degrading mechanical properties ? High residual stress, poor thermal stability and adhesion to the steel substrate. M.W.Moon, Acta Mater., 50 (2002) 1219.
4
Concept of Me-DLC nanocomposite Refractory phases: nc-TiN, TiC, WC, … Primary phases: a-C, C:H, Si 3 N 4 … 2~10 nm ~2nm Hardness: no grain boundary sliding, no dislocations activity, strong interface, strong segregation (immiscibility). Profound effects on the stress, thermal stability, friction coefficient et al !!
5
Previous works C. S. Lee et al., Diamond Rel. Mater. 11 (2002) 198. B. Shi et al, Appl. Phy. Lett. 81(2002)352. B. Feng, Thin Solid Films, 398-399(2001)210 Si atom substitute the carbon atom of sp 3 site. Percolation structure transition from a-C:H like to TiC like occurs.
6
Previous works P. Zhang et al, J. Vac. Sci. Technol. A 20(2002)1390. Increase in sp 2 site and fraction release stress. Due to the absence of hard carbides, soft Al incorporation has a remarkable stress reduction while Ti and Si are inferior. Decrease of mechanical properties in cases of Ti and Si.
7
Motivations Synthesis of WC-C nanocomposite films by hybrid ion beam deposition. Characterization of structure and properties of WC-C films. To examine the role of W on stress reduction. To note the stress reduction origin. To bring forward the generic origin of stress reduction with W incorporation regardless of deposition process.
8
Synthesis process Working gas: Ar, C 6 H 6 (total: 12sccm) Base pressure : 2.0 10 -6 Torr Deposition Pressure : 0.6 ~ 1 10 -4 Torr Power density of target: 4.2~7.3 W/cm 2 RF Bias : - 200 V Thickness: 350±50nm Sputter gun : Third elements addition to DLC (W, Ti, Si …); Ion gun : Easy controlling the ion bombardment energy with high flux. W n+, Ar H +, C m+
9
W composition C Si in substrate Ar W
10
Mechanical properties 1 2 3 21±3 GPa 170±15 GPa
11
Atomic bond structure ?? ** ** The undegrading mechanical properties is related with the unvaired 3-D interlink of atomic bond structure.
12
Role of W on bond structure ?? Region 1 : W essentially act as the relaxation site of nearby carbon network, which is now proposed a generic origin in other W-DLC films. S. J. Park. Diamond Relat. Mater. 11(2002) 1747
13
(c) (d)(e) -W 2 C (101) 2 nm2 nm 2 nm2 nm 2 nm2 nm 4 nm4 nm 4 nm4 nm 4 nm4 nm 4 nm4 nm 4 nm4 nm (e) 4 nm -W 2 C (102) -W 2 C (101) 4 nm (c) -W 2 C (101) 4 nm (b) (a) 4 nm TEM-microstructure changes ?? 4 nm (d) -W 2 C (101) -W 2 C (102) Region 1 : Amorphous carbides formed Region 2 : crystalline carbides begun emerging. Region 3 : crystalline carbides phase presented. (a) 3.0, (b) 4.2, (c) 5.1, (d) 8.7, (d) 12.5 at.% 12 3
14
GIXRD-phase identification ?? 1 2 3 amorphous structure weak crystallinity high crysallinity
15
Region 2: the emergence of crystalline carbides enhanced the distortion of local carbon bond network, which caused the temporary increase in stress. Region 3: the increase in fraction, grain size of the crystalline carbides relief the stress again. 2 3 Stress reduction origins in region 2, 3 The random amorphous network are generally softer than the equivalent crystal one in spite of containing the same atomic bonds. J. Robertson, Mater. Sci. Eng. R 37 (2002) 129.
16
Conclusions WC-C nanocomposite films prepared by hybrid ion beam deposition. The significant stress reduction by W incorporation. The stress is reduced by 50% at 4.2 at.% W, while hardness is only reduced by 20%. W essentially acts as the relaxation site of surrounding carbon network via forming more flexible C-W bond, proposed by a generic origin of stress reduction with W incorporation. Evolution of crystalline carbides plays a subsidiary role on the stress in case of the larger W concentration. W concentration is varied by the Ar fraction in gas mixture.